Procedure - Solid Samples
Instrument calibration/drift correction.
Add approximately 0.05 g of *** Graphite Powder to a *** Graphite Crucible.
Firmly place the crucible on the lower electrode tip or appropriate autoloader position.
Press the Analyze button on the instrument screen, the lower electrode will close and the analysis sequence will start and end automatically.
Repeat steps 3b through 3j a minimum of three times for each calibration/drift standard used.
Calibrate/drift following the procedure outlined in the operator's instruction manual.
Summary
The determination of the amount of oxygen, nitrogen, and hydrogen in iron, steel, nickel-, and cobalt-base alloys represents some of the most important quality metrics for these materials. Oxygen is used to create steel from pig iron by removing excess carbon. Oxygen content must be controlled to limit the amount of carbon monoxide that can be formed during solidification which may cause excessive porosity. Nitrogen is considered both an impurity as well as an important alloying agent. Itcan be present as a nitride or interstitially in its gaseous form. Increased nitrogen content is known to increase yield and tensile strength, thus decreasing ductility and formability. Excessive levels may evolve during solidification thus increasing porosity. High hydrogen content is the primary cause of embrittlement, blistering and flaking due to its high
mobility through the lattice and provides no potential alloying benefits. The ONH836 utilizes a high-power
electrode furnace to quickly and efficiently release the target gases from within the sample, which allows
for a very rapid simultaneous determination of oxygen, nitrogen, and hydrogen.
美国分析仪采购简化日常分析所需的炉头进样部分机械维护工作。
Sample Preparation
Typically, titanium and zirconium samples are chemically etched to remove surface contamination when oxygen and nitrogen are determined. However, etching can introduce hydrogen into the sample.
ASTM method E 1409 "Determination of Oxygen and Nitrogen in Titanium and Titanium Alloys by the Inert
Gas Fusion Technique", as updated in 1996, permits either etching or abrading (filing) of the test specimen.
ASTM E 1447 "Determination of Hydrogen in Titanium and Titanium Alloys by the Inert Gas Fusion Thermal
Conductivity/Infrared Detection Method" permits surface preparation by abrading (if necessary to remove
contamination). Differences in sample preparation present somewhat of a dilemma regarding simultaneous
determination of O, N, and H in titanium. However, abrading samples with a file to remove surface
contamination will yield accurate O, N, and H results. The ONH836 utilizes a high-power electrode furnace to quickly and efficiently release the target gases from within the sample, which allows for a very rapid simultaneous determination of oxygen, nitrogen, and hydrogen.
Procedure - Solid Samples:
--Instrument calibration/drift correction.
Place the nickel basket containing the calibration/drift standard into the open port at the top of the loading head.
Press the Analyze button on the instrument screen again, the loading head slide-block will close and the lower electrode will open.
Clean the upper and lower electrode manually, or, if applicable, remove the crucible and press the analyze button to clean with the automatic cleaner.
ONH836氧氮氢分析仪
高频燃烧红外检测技分析无机材料中的碳、硫含量。
采用惰性气体保护熔融法,提供各种无机材料、钢铁、有色金属、硬质合金、难熔金属、陶瓷等材料中宽范围的氧氮氢同时分析。
该仪器配置MS Windows®的软件接口,专为触摸屏操作定制。长期的开发研究与客户反馈相结合,这个简单方便的软件使得用户可以快速完整访问仪器控制,分析设置,故障诊断,数据报告, **提高日常分析的效率并节省用户宝贵的时间。 可选的Cornerstone® Mobile软件功能,使得用户可以在手机,便携式电脑及台式电脑上便捷的访问仪器数据,分析曲线图形以及仪器的状态,实现对仪器的遥控。
新型气路管道减少气路连接阀,使得漏气,断路故障更少。湖南LECO分析仪咨询报价
***电极炉头设计,提高脉冲炉热交换效率。湖南美国分析仪哪家好
力可ONH836氧氮氢分析仪
特征
稳固的炉头试样加载结构
试样加载过程中完全密闭,消除大气的中可能带来的杂质的污染;
简化日常分析所需的炉头进样部分机械维护工作。
可选的自动功能
上下电极自动清扫装置;
20位试样及坩埚自动进样装置。
附加功能及优点
可选六轴可旋转触摸屏幕,增强了操作的工效和直观性;
可选具有压力补偿和温度控制性能的标气检测气路;
新型气路管道减少气路连接阀,使得漏气,断路故障更少;
配置SmartLine Remote远程诊断功能。
湖南美国分析仪哪家好
上海禹重实业有限公司主要经营范围是仪器仪表,拥有一支专业技术团队和良好的市场口碑。公司业务分为光谱仪,色谱仪,质谱仪,样品前处理等,目前不断进行创新和服务改进,为客户提供良好的产品和服务。公司从事仪器仪表多年,有着创新的设计、强大的技术,还有一批**的专业化的队伍,确保为客户提供良好的产品及服务。禹重科技立足于全国市场,依托强大的研发实力,融合前沿的技术理念,飞快响应客户的变化需求。
氧氮氢分析仪的常见故障及解决方法仪器启动时显示。没有水流。系统分析电流切断,分析停止。这是水流探测器...
【详情】736Series:Oxygen/NitrogenbyInertGasFusionThe736fam
【详情】美国LECO力可氧氮氢分析仪ONH836氧氮氢联测仪系列软件部分1、用户友好界面的Cornersto...
【详情】Procedure–Powder/ChipSamplesInstrumentcalibration/...
【详情】LECO—YoursourcefortotalanalyticalsolutionsCSCS844a...
【详情】InstrumentHighlightsandFeaturesFeaturesandBenefits
【详情】仪器的亮点和优势:特点和优势·炉头区域LED照明系统·炉头快速拆装的粉尘过滤装置·装有自动旁路阀的可...
【详情】Procedure–Powder/ChipSamplesDeterminetheinstrument...
【详情】氧氮氢分析仪的常见故障及解决方法供电正常、通讯正常,点击确认键后分析仪不工作。这是没有水流,炉子温度...
【详情】